摘要:

QFR-2型钩尾框是一种出口铁路车辆的关键部件,借鉴8000 t摩擦压力机的生产经验,对QFR-2型钩尾框在500 kJ对击锤生产重新进行工艺分析,并制定了抬高尾部分模面和挂耳一体锻造的优化工艺方案。采用常温拉伸和高温压缩实验,测定了25MnCrNiMoA钢的材料常数和流变应力曲线,并导入Deform-3D软件,对制定的方案进行有限元分析。研究结果表明,优化后的方案更有利于金属的变形,可以减少打击次数,减少7道加工工序,使废品率从12%降低至3%,从而提高了设备使用寿命,降低了生产成本。

The QFR-2 type of yoke is a key component for export railway vehicles. Therefore, according to the production experience of 8000 t friction press, the process of QFR-2 type of yokes produced by 500 kJ impact hammer was re-analyzed, and the optimized process of raising the die face of tail part and forging lugs integrally was proposed. Then, the material parameters and the flow stress curves were obtained by room temperature tensile and hot compression experiments respectively. Furthermore, the Deform-3D software was input, and the proposed process was analyzed by the finite element. The results show that the optimized process is more conducive to metal deformation. It can reduce the number of blows and seven processing steps so as to decrease the scrap rate from 12% to 3%. Thus, the equipment life can be improved and the cost on production is reduced.

基金项目:
作者简介:
王凯(1973-),男,学士,高级工程师
参考文献:

[1]蒋鹏,付殿禹,曹飞,等. 铁路货车钩尾框精密辊锻过程数值模拟[J].锻压技术,2007,32(3):107-110.Jiang P, Fu D Y, Cao F, et al. FEM analysis of precision roll forging process for train coupler yokes [J].Forging & Stamping Technology, 2007,32(3):107-110.
[2]付殿禹,郑乐启,蒋鹏,等.17型锻造钩尾框热弯曲成形过程数值模拟[J].锻压技术,2009,34(3):22-25.Fu D Y, Zheng L Q, Jiang P, et al. FEM analysis of hot bending process for 17 type of coupler yokes[J].Forging & Stamping Technology, 2009,34(3):22-25.
[3]张鸿斋,朱建军,马利民.列车提速重载对铁路货车的影响[J].铁道车辆,2006,(1):18-24.Zhang H Z, Zhu J J, Ma L M. The influence of train speed increase and heavy load on railway[J].Railway Vehicles,2006,(1):18-24.
[4]唐振英,唐林,赵增华,等.铁路货车锻造钩舌成形工艺及数值模拟优化[J].锻压技术,2012,37(3):11-14.Tang Z Y, Tang L, Zhao Z H, et al. Forging process and FEM optimization for forged knuckles of railway wagons[J].Forging & Stamping Technology, 2012,37(3):11-14.
[5]张志文.锻造工艺学[M].北京:机械工业出版社,1983.Zhang Z W. Forging Technology[M].Beijing: China Machine Press,1983.
[6] 吕炎,江国屏,吴听松,等.锻模设计手册[M].北京:机械工业出版社,2006.Lyu Y, Jiang G P, Wu T S, et al. Forging Die Design Manual[M].Beijing: China Machine Press,2006.
[7]胡建军,李小平.DEFORM-3D塑性成形CAE应用教程[M].北京:北京大学出版社,2011.Hu J J, Li X P. DEFORM-3D Plastic Forming CAE Application Tutorial[M] .Beijing: Peking University Press,2011.
[8]于秋华,刘淑梅,刘雅辉,等.基于Deform-3D的曲轴热锻工艺参数优化[J].锻压技术,2015,40(3):131-135.Yu Q H, Liu S M, Liu Y H, et al. Optimization of hot forging process parameters of crankshaft based on Deform-3D[J]. Forging & Stamping Technology,2015,40(3):131-135.
服务与反馈:
文章下载】【加入收藏
《锻压技术》编辑部版权所有

中国机械工业联合会主管  中国机械总院集团北京机电研究所有限公司 中国机械工程学会主办
联系地址:北京市海淀区学清路18号 邮编:100083
电话:+86-010-82415085 传真:+86-010-62920652
E-mail: fst@263.net(稿件) dyjsjournal@163.com(广告)
京ICP备07007000号-9