Abstract:
|
Fracture cracks are generated at the bottom beam of extruding press,which losses its functions and needs to be repaired.Being repositioned with home-made self-locking hydraulic puller device,the carbon dioxide gas arc welding and DC arc welding were made on the top,bottom and side parts of the fracturing crack.The warm-up before welding,heat holding during welding,low temperature tempering after welding and vibrating and hitting operation after every welding layer were used to eliminate the welding stress.After welding repair,active beam function was restored.It proves that it can meet the requirement of the extruding press through the application experiences for several years.
|