Abstract:
|
Three quarter die forgings were broken along parting line among 150 forgings of Ф550mm traveling crane wheels forged on drop hammer of 16t.The warp flash was produced and some of them were remained after trimming.The forging procedure tracing and parting face structure analyzing were performed.The result shows that wheel breaking along parting line is caused by trimming flash.Forging offset causes error repairing pattern.The main reason is the impression offset in forging which causes bigger trimming width and force.
|
Funds:
|
|
AuthorIntro:
|
|
Reference:
|
[1]锻件质量分析编写组.锻件质量分析[M].北京:机械工业出版社,1983.
[2]王仲仁.锻压手册(锻造第3卷)[M].北京:机械工业出版社,2002.
[3]吕炎.锻造缺陷分析与对策[M].北京:机械工业出版社,1999.
[4]吕炎.锻造工艺学[M].北京:机械工业出版社,1995.
[5]万煦义.提高大中型柴油机连杆模锻件质量的途径[J].锻压技术,2006,31(3):4-8.
|